Table 1 |
||||||||||
|
Physical and electrical properties of (1-x)BNKT-xBST ceramics sintered at 1,125°C |
||||||||||
|
x |
Density (g/cm3) |
c/a |
Grain size (μm) |
Tc (°C) |
εra |
tanδa |
Pr (μC/cm2) |
Ec (kV/cm) |
Rsq |
d33 (pC/N) |
|
|
||||||||||
|
0 |
5.81 ± 0.01 |
1.0083 |
0.60 ± 0.09 |
320 |
1,419 |
0.0479 |
31.62 |
32.01 |
1.12 |
178 |
|
0.05 |
5.80 ± 0.02 |
1.0118 |
0.40 ± 0.04 |
310 |
1,581 |
0.0559 |
14.03 |
10.28 |
0.48 |
98 |
|
0.10 |
5.77 ± 0.01 |
1.0120 |
0.39 ± 0.04 |
308 |
1,609 |
0.0618 |
28.14 |
22.96 |
1.04 |
214 |
|
0.15 |
5.76 ± 0.01 |
1.0156 |
0.46 ± 0.07 |
305 |
1,430 |
0.0576 |
25.11 |
25.67 |
0.98 |
205 |
|
0.20 |
5.72 ± 0.01 |
1.0163 |
0.47 ± 0.06 |
289 |
1,082 |
0.0477 |
21.96 |
29.08 |
0.98 |
191 |
|
|
||||||||||
|
aDielectric data obtained at room temperature (1 kHz). |
||||||||||
|
Jaita et al. Nanoscale Research Letters 2012 7:24 doi:10.1186/1556-276X-7-24 |
||||||||||