Table 1 |
|||||
|
Major shape distribution of AuNPs at different experimental conditions |
|||||
|
Concentration of gold salt (mM)/detergent (wt.%) |
Temperature (°C) |
Shape distribution (%) |
|||
|
Triangular |
Spherical |
Pentagonal |
Hexagonal |
||
|
|
|||||
|
0.4/1 |
25 |
44.8 |
42.0 |
6.4 |
5.5 |
|
0.4/10 |
25 |
1.3 |
97.4 |
0.7 |
0.7 |
|
0.4/25 |
25 |
0.6 |
95.3 |
1.4 |
2.7 |
|
1/1 |
25 |
18.1 |
14.3 |
46.6 |
19.6 |
|
0.4/1 |
4 |
76.8 |
7.1 |
5.4 |
10.7 |
|
0.4/1 |
45 |
25.8 |
57.9 |
14.7 |
1.6 |
|
0.4/1 |
65 |
6.1 |
69.3 |
6.8 |
2.7 |
|
|
|||||
|
Premkumar et al. Nanoscale Research Letters 2011 6:547 doi:10.1186/1556-276X-6-547 |
|||||