Table 1 |
|||||
| SSA and deNOxability of the samples prepared under different conditions, together with those of P25 titania | |||||
| Sample | Synthesis condition | Morphology | SSA (m2/g) | DeNOxphotocatalytic activity (%) | |
| >410 nm | >290 nm | ||||
| P25 Titania AEROXIDE® | Commercial | – | 55.9 | 28.3 | 37.5 |
| ZnO | 0.01 M ZnCl2–HMT mixed aqueous solution | Spindle-like | 4.3 | 4.25 | 18.1 |
| Zn5(OH)8Cl2 · H2O | 0.05 M ZnCl2–HMT mixed aqueous solution | Plate-like | 19.4 | 2.01 | 11.7 |
| ZnO | 0.05 M ZnCl2–HMT mixed 50% EG solution | Hexagonal rod-like | 3.2 | 0 | 17.7 |
| Zn5(OH)8Cl2 · H2O | 0.1 M ZnCl2–HMT mixed 50% EG solution | Plate-like | 19.7 | 0 | 11.2 |
Long et al. Nanoscale Research Letters 2008 4:247 doi:10.1186/1556-276X-4-247